Aluminium Alloys – Material Properties
Aluminium alloys are used for structural members where low self-weight, corrosion resistance and easy extrusion are decisive: facades and curtain walls, roofs, footbridges, masts, towers, temporary structures and long-span roofs. Unlike steel, aluminium is not a single material — the resistance depends on the alloy (EN AW-6xxx, 5xxx, 7xxx series) and on the temper (O, T4, T5, T6, T66, H111, H12 ...), i.e. on the heat treatment or cold working condition of the product.
The design values are defined by EN 1999-1-1 (Eurocode 9 – Design of aluminium structures). This page summarises the material constants given in EN 1999-1-1 §3.2.5 and the characteristic values of the 0.2 % proof strength f0 and of the ultimate tensile strength fu given in EN 1999-1-1 Table 3.2b for extruded profiles, extruded tube, extruded rod/bar and drawn tube, which are the product forms used in structural work.
The mechanical properties are taken from the product standards EN 755-2 (extruded rod/bar, tube and profiles), EN 754-2 (cold drawn rod/bar and tube) and EN 485-2 (sheet, strip and plate). The values below are valid for service temperatures up to 80 °C; the alloy and temper designations follow EN 573-3.
Design values of the material constants
The material constants to be adopted in calculations are given in EN 1999-1-1 §3.2.5:
| Property | Symbol | Value | Unit |
|---|---|---|---|
| Density | ρ | 2700 | kg/m3 |
| Modulus of elasticity (Young's modulus) | E | 70 000 | N/mm2 |
| Shear modulus | G | 27 000 | N/mm2 |
| Poisson's ratio in the elastic range | ν | 0.30 | – |
| Coefficient of linear thermal expansion | α | 23 ×10-6 | K-1 |
| Partial factor – resistance of cross-sections | γM1 | 1.10 | – |
| Partial factor – members to instability, tension to fracture | γM2 | 1.25 | – |
The modulus of elasticity of aluminium is about one third of that of steel (70 000 N/mm2 compared with 210 000 N/mm2), a fact that governs the design: aluminium members are usually limited by deformation and by stability rather than by the resistance of the cross-section.
Characteristic values of f0 and fu – extruded and drawn products
EN 1999-1-1 Table 3.2b – characteristic values of the 0.2 % proof strength f0, ultimate tensile strength fu, minimum elongation A and buckling class for the most common structural alloys. Product forms: EP – extruded profiles (EP/O open, EP/H hollow), ET – extruded tube, ER/B – extruded rod/bar, DT – drawn tube.
| Alloy | Temper | Product form | Thickness t [mm] | f0 [N/mm2] | fu [N/mm2] | A [%] | Buckling class |
|---|---|---|---|---|---|---|---|
| EN AW-6060 | T5 | EP, ET, ER/B | t ≤ 5 | 120 | 160 | 8 | B |
| EN AW-6060 | T5 | EP | 5 < t ≤ 25 | 100 | 140 | 8 | B |
| EN AW-6060 | T6 | EP, ET, ER/B | t ≤ 3 | 160 | 215 | 8 | A |
| EN AW-6060 | T6 | EP, ET, ER/B | 3 < t ≤ 15 | 140 | 170 | 8 | A |
| EN AW-6063 | T5 | EP, ET, ER/B | t ≤ 3 | 130 | 175 | 8 | B |
| EN AW-6063 | T5 | EP | 3 < t ≤ 25 | 110 | 160 | 7 | B |
| EN AW-6063 | T6 | EP, ET, ER/B | t ≤ 25 | 160 | 195 | 8 | A |
| EN AW-6061 | T4 | EP, ET, ER/B | t < 25 | 110 | 180 | 15 | B |
| EN AW-6061 | T6 | EP, ET, ER/B | t < 25 | 240 | 260 | 8 | A |
| EN AW-6005A | T6 | EP/O, ER/B | t ≤ 5 | 225 | 270 | 8 | A |
| EN AW-6005A | T6 | EP/O, ER/B | 5 < t ≤ 10 | 215 | 260 | 8 | A |
| EN AW-6005A | T6 | EP/O, ER/B | 10 < t ≤ 25 | 200 | 250 | 8 | A |
| EN AW-6005A | T6 | EP/H, ET | t ≤ 5 | 215 | 255 | 8 | A |
| EN AW-6005A | T6 | EP/H, ET | 5 < t ≤ 10 | 200 | 250 | 8 | A |
| EN AW-6082 | T4 | EP, ET, ER/B | t ≤ 25 | 110 | 205 | 14 | B |
| EN AW-6082 | T5 | EP | t ≤ 5 | 230 | 270 | 8 | B |
| EN AW-6082 | T6 | EP | t ≤ 5 | 250 | 290 | 8 | A |
| EN AW-6082 | T6 | ET | 5 < t ≤ 15 | 260 | 310 | 10 | A |
| EN AW-6082 | T6 | ER/B | 20 < t ≤ 50 | 260 | 310 | 8 | A |
| EN AW-6082 | T6 | DT | t ≤ 20 | 240 | 310 | 10 | A |
| EN AW-5083 | O | EP, ET, ER/B | t ≤ 200 | 110 | 270 | 12 | B |
| EN AW-5083 | H12/H22/H32 | EP, ET, ER/B | t ≤ 10 | 200 | 280 | 6 | B |
| EN AW-5754 | O/H111 | EP, ET, ER/B | t ≤ 25 | 80 | 180 | 14 | B |
| EN AW-5454 | O/H111 | ET, F/H112 | t ≤ 25 | 85 | 200 | 16 | B |
| EN AW-7020 | T6 | EP, ET, ER/B | t ≤ 15 | 290 | 350 | 10 | A |
| EN AW-7020 | T6 | EP, ET, ER/B | 15 < t < 40 | 275 | 350 | 10 | A |
Welded members – heat affected zone (HAZ)
Welding reduces the strength of the material in the heat affected zone. EN 1999-1-1 accounts for this with the reduced characteristic values f0,haz and fu,haz (also tabulated in Table 3.2b) or, equivalently, with the reduction factors ρ0,haz = f0,haz / f0 and ρu,haz = fu,haz / fu. For the 6xxx and 7xxx alloys (precipitation hardening) the loss of strength is important — for example ρ0,haz is about 0.50–0.60 for 6082 T6 and about 0.42–0.50 for 6060 T5 — while for the 5xxx alloys in the O condition there is no reduction at all.
- The HAZ values given in the standard are valid for MIG welding and thicknesses up to 15 mm. For TIG welding of precipitation hardening alloys up to 6 mm they shall be multiplied by 0.8, and for greater thicknesses a further reduction applies (0.8 for 6xxx/7xxx alloys, 0.9 for 3xxx/5xxx alloys), except in temper O.
- The mechanical properties recover with time after welding: 3 days for the 6xxx alloys and 30 days for the 7xxx alloys, provided that the material is kept at a temperature of at least 10 °C.
- For service temperatures between 80 °C and 100 °C the characteristic strengths shall be reduced; at 100 °C, k100 = 0.1 for strain hardening alloys (3xxx, 5xxx) and k100 = 0.2 for precipitation hardening alloys (6xxx, 7020).
- Buckling class A or B is used in the member verification (EN 1999-1-1 §6.3.1); most 6xxx alloys in tempers T5/T6 fall in class A, the softer tempers and the 5xxx alloys in class B.
- Aluminium is not covered by EN 1993; the resistance formulae, the classification of cross-sections (four classes) and the buckling curves are specific to EN 1999-1-1 and differ from those of steel.
- The modulus of elasticity does not depend on the alloy or temper, so the deflections of members of the same geometry are practically the same for all alloys — only the resistance changes.