Copper – Material Properties


Copper is one of the oldest materials used in construction and remains the reference material for roof coverings, wall cladding, rainwater goods (gutters and downpipes), flashings and architectural details. Its use is based on three properties: excellent corrosion resistance (the surface develops a protective patina of basic copper salts), very long service life — 80 to 100 years and more for roofing — and simple, cold-forming workmanship with traditional metal-working tools.

The wrought products for building applications are covered by EN 1172 (copper and copper alloys – sheet and strip for the construction industry) and EN 13599 (copper plate, sheet and strip), while the roofing products themselves are specified in EN 504 (fully supported roofing elements) and EN 506 (self-supporting roofing elements). The grades normally used are Cu-ETP (CW004A, 2.0060) and Cu-DHP (CW024A, 2.0090), both with a copper content of at least 99.90 %.

It should be noted that there is no European design code for copper structures (unlike EN 1993 for steel and EN 1999 for aluminium). The values below are the mechanical properties guaranteed by the product standards, used as characteristic values; the partial safety factors for a structural verification have to be agreed for each project (values of the order of γM = 1.1 to 1.5 are typical, depending on the consequence class and on the quality control). For roof and facade elements, copper is in most cases a non-structural or secondary element, and its design is governed by fixing and thermal movement rather than by resistance.

Physical properties

PropertySymbolValueUnit
Densityρ8.9 – 9.0 (typically 8.96)kg/dm3
Modulus of elasticity (Young's modulus)E110 – 130 (≈ 115)GPa
Shear modulusG = E / [2·(1+ν)]≈ 43GPa
Poisson's ratio in the elastic rangeν0.34–
Coefficient of linear thermal expansion (20 – 300 °C)α17 ×10-6K-1
Thermal conductivity (20 °C)λ390W/(m·K)
Electrical conductivity–100% IACS
Melting range–1070 – 1083°C
Modulus of elasticity – cold worked materialEup to ≈ 130GPa

The modulus of elasticity of copper depends on the degree of cold working: about 110 GPa in the soft (annealed) condition and up to about 130 GPa in the hard condition. For the usual architectural applications the value E ≈ 115 GPa is used.

Mechanical properties – tempers according to EN 1172

The temper is designated by R followed by the minimum tensile strength in N/mm2 (e.g. R240 means Rm ≥ 240 N/mm2). The values below are the minimum values of the product standard; the ranges apply to the thicknesses usually delivered for roofing and cladding.

TemperConditionThickness [mm]Rm [N/mm2]Rp0.2 [N/mm2]A50 [%]Hardness HV
R220soft / annealed0.10 – 5220 – 260≤ 140≥ 3340 – 65
R240half hard0.10 – 10240 – 300≥ 180≥ 865 – 95
R290hard0.10 – 10290 – 360≥ 250≥ 490 – 110

A harder temper (R360) is also produced for special applications: Rm ≥ 360 N/mm2, Rp0.2 ≥ 320 N/mm2, A50 ≥ 2 %, hardness ≥ 110 HV.

Notes