Structural Steel – Material Properties
Structural steel is the most widely used material for load-bearing structures, and its design values in the European Union are defined by EN 1993-1-1 (Eurocode 3 – Design of steel structures) together with the product standards for the individual product forms. This page summarises the design values of the material coefficients (elastic modulus, shear modulus, Poisson's ratio, thermal expansion, density) and the nominal values of the yield strength fy and of the ultimate tensile strength fu given in EN 1993-1-1 Table 3.1, which form the basis of every cross-section and member verification.
The nominal strengths depend on the steel grade and on the nominal thickness of the element t: for thicker elements the values are lower, because both the cooling rate after rolling and the amount of deformation are smaller. Table 3.1 covers two thickness ranges (t ≤ 40 mm and 40 mm < t ≤ 80 mm); for thicker products the values shall be taken from the relevant product standard or from the National Annex.
The grades are defined in the product standards: EN 10025-2 (hot rolled non-alloy structural steels), EN 10025-3 (normalized / normalized rolled weldable fine grain steels), EN 10025-4 (thermomechanically rolled weldable fine grain steels), EN 10025-5 (structural steels with improved atmospheric corrosion resistance) and EN 10025-6 (quenched and tempered steels). Structural hollow sections are covered by EN 10210-1 (hot finished) and EN 10219-1 (cold formed).
Design values of the material coefficients
The material constants to be adopted in calculations are given in EN 1993-1-1 §3.2.6. The unit weight is taken from EN 1991-1-1 Table A.4, which gives values between 77.0 and 78.5 kN/m3; in practice γ = 78.5 kN/m3 (ρ ≈ 7850 kg/m3) is used.
| Property | Symbol | Value | Unit |
|---|---|---|---|
| Density | ρ | 7850 | kg/m3 |
| Unit weight | γ | 78.5 | kN/m3 |
| Modulus of elasticity (Young's modulus) | E | 210 000 | N/mm2 |
| Shear modulus | G = E / [2·(1+ν)] | 81 000 | N/mm2 |
| Poisson's ratio in the elastic range | ν | 0.30 | – |
| Coefficient of linear thermal expansion (T ≤ 100 °C) | α | 12 ×10-6 | K-1 |
| Coefficient of linear thermal expansion for composite structures | αc | 10 ×10-6 | K-1 |
| Minimum elongation at failure | A | ≥ 15 | % |
| Minimum ratio of the strengths | fu / fy | ≥ 1.10 | – |
Nominal values of fy and fu – hot rolled structural steel
EN 1993-1-1 Table 3.1 – nominal values of the yield strength fy and of the ultimate tensile strength fu for hot rolled structural steel.
| Standard | Steel grade | fy [N/mm2] t ≤ 40 mm | fu [N/mm2] t ≤ 40 mm | fy [N/mm2] 40 < t ≤ 80 mm | fu [N/mm2] 40 < t ≤ 80 mm |
|---|---|---|---|---|---|
| EN 10025-2 | S 235 | 235 | 360 | 215 | 360 |
| EN 10025-2 | S 275 | 275 | 430 | 255 | 410 |
| EN 10025-2 | S 355 | 355 | 510 | 335 | 470 |
| EN 10025-2 | S 450 | 440 | 550 | 410 | 550 |
| EN 10025-3 | S 275 N/NL | 275 | 390 | 255 | 370 |
| EN 10025-3 | S 355 N/NL | 355 | 490 | 335 | 470 |
| EN 10025-3 | S 420 N/NL | 420 | 520 | 390 | 520 |
| EN 10025-3 | S 460 N/NL | 460 | 540 | 430 | 540 |
| EN 10025-4 | S 275 M/ML | 275 | 370 | 255 | 360 |
| EN 10025-4 | S 355 M/ML | 355 | 470 | 335 | 450 |
| EN 10025-4 | S 420 M/ML | 420 | 520 | 390 | 500 |
| EN 10025-4 | S 460 M/ML | 460 | 540 | 430 | 530 |
| EN 10025-5 | S 235 W | 235 | 360 | 215 | 340 |
| EN 10025-5 | S 355 W | 355 | 510 | 335 | 490 |
| EN 10025-6 | S 460 Q/QL/QL1 | 460 | 570 | 440 | 550 |
Nominal values of fy and fu – structural hollow sections
EN 1993-1-1 Table 3.1 (continued) – the same nominal values for hot finished (EN 10210-1) and cold formed (EN 10219-1) structural hollow sections. For cold formed hollow sections the standard lists values only for t ≤ 40 mm.
| Standard | Steel grade | fy [N/mm2] t ≤ 40 mm | fu [N/mm2] t ≤ 40 mm | fy [N/mm2] 40 < t ≤ 80 mm | fu [N/mm2] 40 < t ≤ 80 mm |
|---|---|---|---|---|---|
| EN 10210-1 | S 235 H | 235 | 360 | 215 | 340 |
| EN 10210-1 | S 275 H | 275 | 430 | 255 | 410 |
| EN 10210-1 | S 355 H | 355 | 510 | 335 | 490 |
| EN 10210-1 | S 275 NH/NLH | 275 | 390 | 255 | 370 |
| EN 10210-1 | S 355 NH/NLH | 355 | 490 | 335 | 470 |
| EN 10210-1 | S 420 NH/NLH | 420 | 540 | 390 | 520 |
| EN 10210-1 | S 460 NH/NLH | 460 | 560 | 430 | 550 |
| EN 10219-1 | S 235 H | 235 | 360 | – | – |
| EN 10219-1 | S 275 H | 275 | 430 | – | – |
| EN 10219-1 | S 355 H | 355 | 510 | – | – |
| EN 10219-1 | S 275 NH/NLH | 275 | 370 | – | – |
| EN 10219-1 | S 355 NH/NLH | 355 | 470 | – | – |
| EN 10219-1 | S 460 NH/NLH | 460 | 550 | – | – |
| EN 10219-1 | S 275 MH/MLH | 275 | 360 | – | – |
| EN 10219-1 | S 355 MH/MLH | 355 | 470 | – | – |
| EN 10219-1 | S 420 MH/MLH | 420 | 500 | – | – |
| EN 10219-1 | S 460 MH/MLH | 460 | 530 | – | – |
Partial safety factors
The partial factors γM are applied to the characteristic (nominal) values of the resistance. The values recommended in EN 1993-1-1 §6.1 are:
| Partial factor | Value | Applied to |
|---|---|---|
| γM0 | 1.00 | resistance of cross-sections, whatever the class |
| γM1 | 1.00 | resistance of members to instability (buckling) |
| γM2 | 1.25 | resistance of cross-sections in tension to fracture and connections |
Notes
- The values of fy and fu in Table 3.1 are nominal values; they are used directly in the resistance formulae together with the partial factors γM0 and γM1.
- A lower thickness of the element gives a higher strength. For the same grade the value to be used is the one of the thickness range in which the element falls (e.g. S 355: 355 N/mm2 for t ≤ 40 mm, 335 N/mm2 for 40 < t ≤ 80 mm).
- The suffixes N/NL, M/ML and Q/QL indicate the delivery condition (normalized, thermomechanically rolled, quenched and tempered) and the impact test temperature (L = low temperature, −50 °C).
- The impact toughness is defined by the sub-grade of the steel: JR – 27 J at +20 °C, J0 – 27 J at 0 °C, J2 – 27 J at −20 °C, K2 – 40 J at −20 °C. The choice of the sub-grade is made according to EN 1993-1-10.
- The values in this table are valid for service temperatures up to 100 °C. For fire design see EN 1993-1-2, which gives reduction factors for the yield strength and for the modulus of elasticity at elevated temperatures.
- The 210 000 N/mm2 modulus of elasticity is a nominal value used for all grades; E does not depend on the steel grade.